Chinese name | Grade |
alloy element% |
use |
Add amount |
Use temperature °C |
performance |
ALCu |
ALCu50 |
Cu48~52 |
Adjust alloy composition |
Depends on demand |
570~600 |
brittle |
AlSi |
ALSi20 |
Si18~20 | Adjust alloy composition | Depends on demand |
700~800 | brittle |
ALMn |
ALMn10 |
Mn9~11 | Adjust alloy composition | Depends on demand |
770~830 |
tough |
ALMn |
ALMn20 |
Mn18~22 | Adjust alloy composition | Depends on demand |
780~850 | tough |
ALTi |
ALTi5 |
Ti4~6 | Grain refinement, improve plasticity | Depends on demand |
1020~1070 | Easy segregation |
ALTi |
ALTi10 |
Ti9~11 | Grain refinement, improve plasticity | Depends on demand |
1020~1070 | Easy segregation |
ALTi | ALTi10
|
Ni9~11 | Improve plasticity | Depends on demand |
680~730 |
tough |
ALCr |
ALCr5 |
Cr4~6 | Improve plasticity, improve performance | Depends on demand |
900~1000 | Easy segregation |
ALCr |
ALCr10 |
Cr9~11 | Improve plasticity, improve performance | Depends on demand |
900~1000 | Easy segregation |
ALCr |
ALCr20 |
Cr18~22 | Improve plasticity, improve performance | Depends on demand |
910~1020 | Easy segregation |
ALZr |
ALZr5 |
Zr4~6 | Improve plasticity, improve performance | Depends on demand |
800~850 | Easy segregation |
ALSb |
ALSb4 |
Sb3~5 | Improve plasticity, improve performance | Depends on demand |
660 | Easy segregation |
ALSb |
ALSb10 |
Sb9~11 | Improve plasticity, improve performance | Depends on demand |
660 | Easy segregation
|
ALFe |
ALFe20 |
Fe18~22 | Improve plasticity, improve performance | Depends on demand |
1020 |
brittle |
ALBe |
ALBe1 |
Be0.9~1.2 | Improve plasticity, improve performance | Depends on demand |
820 |
tough |
ALBe |
ALBe3 |
Be2~4 | Improve plasticity, improve performance | Depends on demand |
820 |
tough |
ALBe |
ALBe5 |
Be4.5~5.5 | Improve plasticity, improve performance | Depends on demand |
820 |
tough |
ALB |
ALB3 |
B2.5~3.5 | Reduce resistivity, improve conductivity, and refine grain |
2~4% |
800 |
tough |
ALTi5B |
ALTi5B1 |
Ti4.5~6 B0.9~1.2 | Grain Refinement |
0.5~2‰ |
800 | Easy segregation |
ALRe |
ALRe10 |
Re9~11 | Grain Refinement | 2~3‰
|
680 | Easy segregation |
ALTi5B1Re |
ALTi5B1Re10 |
Ti5B1Re10 | Grain Refinement | 1~3‰
|
800 | Easy segregation |
ALTi5C0 |
ALTi5C0.2 |
Ti5C0.2 | Grain Refinement | 1~2‰
|
1020~1070 | Easy segregation |
ALSr |
ALSr10 |
Sr9~11 | For long-term deterioration of aluminum-silicon alloys with silicon below 13% | 1~2‰
|
680~740 | Easy segregation |
ALY |
ALY5 |
Y4~6 |
Improve plasticity and increase fluidity | 1~2‰
|
740~800 | Easy segregation |
ALBi |
ALBi10 |
Bi9~11 |
Improve plasticity and increase fluidity | 1~2‰
|
700~710 | Easy segregation |
ALSc |
ALSc2 |
Sc |
Adjust alloy composition,Improve alloy properties | Depends on demand |
700-800 | tough |
ALCo |
ALCo5 |
Co |
Adjust alloy composition,Improve alloy properties | Depends on demand |
720-750 | tough |
ALMo5 |
ALMo5-10 |
Mo |
Adjust alloy composition,Improve alloy properties | Depends on demand |
720-750 | tough |
ALNb |
ALNb10 |
Nb |
Increase fluidity and improve alloy properties | Depends on demand |
690-750 | tough |
ALNd |
ALNd30 |
Nd |
Adjust alloy composition,Improve alloy properties | Depends on demand |
690-750 | Easy segregation |
ALCe |
ALCe10 |
Ce |
Adjust alloy composition,Improve alloy properties | Depends on demand |
690-750 | Easy segregation |
ALCd5 |
ALCd5 / 10 |
Cd |
Adjust alloy composition,Improve alloy properties | Depends on demand |
690-750 | tough |
ALTe |
ALTe5 |
Te |
Adjust alloy composition,Improve alloy properties | Depends on demand |
710-740 | brittle |
The chemical composition and impurities of aluminum master alloy ingots are produced according to the YS/T282-2000 standard, and other master alloys and casting alloys can be produced according to user needs. |